Home » Insights » 7075-T6 vs T73/T7351 for CNC Parts: Choosing the Right Temper

7075-T6 vs T73/T7351 for CNC Parts: Choosing the Right Temper

Dewey Wu, General Manager at EPOC CRAFTER

Dewey Wu General Manager & senior mechanical engineer at EPOC CRAFTER, 15 years in design engineering, quality, and metallurgy. Hands-on across CNC machining, metalwork, sheet metal, and prototyping (subtractive + 3D printing).

Dewey Wu on LinkedIn

7075 T6 aluminum offers high strength, but it is not always the right choice for CNC parts. T73 prioritizes resistance to stress corrosion cracking, while T651 and T7351 add stress relief through stretching to their respective heat treatment conditions. Your choice depends on service exposure, required strength, stock form, part geometry, machining sequence, and inspection requirements. A stress-relieved temper does not guarantee that a heavily machined part will remain flat after unclamping.

This article addresses temper selection within 7075. The separate 6061 vs 7075 aluminum selection guide covers the earlier choice between alloys. The broader 6061 vs 7075 aluminum selection covers the alloy-level choice.

1. Understanding 7075 Aluminum Tempers: T6, T651, T73, and T7351

7075-T6, T651, T73 and T7351 are conditions of the same alloy, not different grades. The first decision is whether higher specified strength or improved resistance to stress corrosion cracking controls the application. The second is whether stretched, stress-relieved stock suits the machining route. Neither choice removes the need to check the applicable product specification.

TemperMaterial conditionMain engineering consideration
7075-T6Solution heat treated and artificially agedHigher specified strength, with SCC susceptibility requiring attention
7075-T651T6 condition with stress relief by stretchingHigher specified strength combined with stress-relieved stock
7075-T73Solution heat treated and overagedGreater SCC resistance under relevant conditions, with lower specified strength
7075-T7351T73 condition with stress relief by stretchingT73-type SCC requirements combined with stress-relieved stock

Temper designations follow the Aluminum Association system. Actual mechanical property requirements depend on the applicable material specification, product form, and dimensions. The broader 6061 T6 vs T651 temper differences article concerns another alloy and should not be used to substitute 6061 temper rules for 7075.

These 7075 aluminum tempers solve different design problems. 7075 T6 aluminum is often specified for its high strength. 7075 T651 aluminum adds stretching for stress relief, while 7075 T73 aluminum is an overaged condition with different SCC requirements. The terms T6 vs T651 and 7075 T6 vs T651 describe a processing distinction, not a new alloy. Likewise, 7075 T73 vs T7351 compares overaged material with its stretched counterpart.

The 7075 aluminum alloy is widely used where strength and weight both matter. Still, 7075 aluminum properties cannot be inferred from the alloy number alone. In a temper comparison, check the production form, section thickness and qualification requirements before treating nominal values as purchasing limits.

1.1. T6 vs T73: Strength and Stress Corrosion Resistance

The difference between 7075 T6 vs T73 becomes important when a component operates under sustained tensile stress in an environment capable of promoting stress corrosion cracking. T6 is attractive where high specified yield strength matters. T73 sacrifices some specified strength to provide greater SCC resistance under relevant test conditions.

ASTM B211/B211M-23 provides a comparison for covered rolled or cold-finished 7075 products with specified thickness or diameter greater than 3.20 mm and up to 100.00 mm:

Specification minimumT6/T62T73/T7351
Tensile strength530 MPa470 MPa
0.2% offset yield strength455 MPa425 MPa
Elongation, 50 mm gauge length7%10%

Source: ASTM B211/B211M-23, Table 3. These values are specification limits for the covered products and conditions, not measured averages or universal properties of 7075 plate and extrusion. The 7075 aluminum yield strength difference affects material design allowables, not the verified load capacity of a bracket, housing, or complete assembly. Hole geometry, remaining sections, contact pressure, fatigue loading, and service conditions still require evaluation.

ASTM G47-26 evaluates SCC susceptibility under specified test conditions. Meeting material requirements does not guarantee that a finished component will resist cracking throughout its service life.

1.2. T651 vs T7351: What Stress Relief Actually Changes

The comparison between 7075 T651 vs T7351 involves both aging condition and stress relief. T651 retains T6-type strength characteristics while incorporating stretching to reduce residual stress. T7351 combines T73-type aging with stretching. Neither designation specifies a universal residual stress value for every plate thickness, and neither guarantees post-machining flatness.

Consider an actual EPOC CRAFTER production and finished-part inspection case involving a precision instrument housing bracket machined from 7075-T651 rolled plate. The starting blank measured 170 × 120 × 32 mm. The finished part measured 160 × 110 × 25 mm, with local ribs as thin as 2.5 mm and a main cavity 17 mm deep.

The machining route used staged roughing, a second setup, controlled clamping, and final inspection after unclamping and temperature stabilization. Base mounting surface flatness was 0.065 mm against a 0.10 mm limit. Maximum four-hole positional deviation was ⌀0.12 mm against ⌀0.20 mm. Inspection occurred at 20 ± 1°C after at least two hours of stabilization. Both reported geometric results met their stated limits.

These are actual production engineering and finished-part inspection figures supplied by EPOC CRAFTER. The production route used T651 only. It does not establish a measured distortion advantage over T7351 or T6. It shows that stock temper and machining sequence must be considered together, and that this component was accepted in a free state after fixture release. The supplied case identifies AMS4045N as the plate procurement specification; the order and product thickness must be checked against that standard’s applicable scope.

2. Strength Limits Depend on Form, Temper, and Section

A single 7075 aluminum tensile strength figure is not a drawing specification. The minimum depends on temper, stock form, section size and test conditions. Keep material acceptance separate from finished-part load capacity.

ASTM B211/B211M-23 Table 3 sets a minimum T651 tensile strength of 530 MPa for its covered products above 3.20 through 100.00 mm; this falls to 515 MPa above 100.00 through 160.00 mm. Copying the smaller-section figure onto a larger bar would create a false acceptance limit. These B211 numbers do not apply to plate or extrusion.

7075 gains strength through precipitation hardening after solution treatment and aging. Overaging changes its strength and SCC response. Hardness may be useful in process investigation, but it cannot substitute for required tensile tests or SCC acceptance. Material chemistry, heat treatment, stock form and permitted section govern the 7075 aluminum mechanical properties used for design. Review aluminum material properties when comparing materials before choosing a 7075 temper.

For a strength calculation, check 7075 T6 properties and the appropriate 7075 T6 yield strength under the selected product specification. The same caution applies to 7075 T6 tensile strength, 7075 T7351 properties and 7075 T651 properties. A web chart headed 7075 aluminum strength may combine nominal and minimum values; the drawing needs the applicable limits and directions.

7075 aluminum hardness and 7075 T6 hardness may help investigate a process discrepancy, but hardness cannot replace prescribed tensile tests. A 7075 aluminum heat treatment or 7075 heat treatment description must identify the approved processing route. Aluminum precipitation hardening explains why tempers differ, but a high strength aluminum alloy label alone is not an acceptance criterion.

2.1. Do Not Turn a Material Minimum into a Finished-Part Load Rating

The minimum material yield limit does not predict bolt-bearing failure, thread stripping, crack growth or out-of-plane bending. For an aerospace fitting with load across the plate short-transverse direction, thickness orientation and stress concentration can dominate selection. Neither high strength aluminum alloy marketing claims nor an unspecified 7075 aluminum tensile strength is a structural substantiation.

7075 T6 and T73 strength limits by product size.

3. Stress Corrosion Resistance Is a Qualification Question

Stress corrosion cracking depends on alloy condition, sustained tensile stress, exposure and orientation. The 7075-T73 family is selected where its applicable SCC requirements matter; it is not a universal guarantee against cracking.

ASTM B211/B211M-23 section 13 establishes SCC-related requirements for its covered 7075-T73 and T7351 products, including lot acceptance based on electrical conductivity together with mechanical-property conditions. ASTM E1004 governs the referenced conductivity test method. Applicable thicker products also undergo the specified short-transverse SCC verification under ASTM G47 conditions. The B211/B211M-23 technical extract identifies 20.00 mm and above, loading at 75% of specified minimum yield strength and no visually evident SCC as the stated verification context. Verify the matching product specification before extending these conditions to plate or extrusions.

ASTM G47-26 specifies a laboratory procedure using an alternate-immersion 3.5% NaCl environment to characterize SCC susceptibility of relevant wrought alloys. The ASTM scope explicitly calls for additional service-representative testing when actual serviceability must be established. Thus the correct question is not simply, “Is 7075 aluminum corrosion resistant?” It is whether the product, stress direction, exposure, protective coating and qualification evidence match the intended service.

The term 7075 stress corrosion cracking describes a specific failure concern, not all corrosion. For aluminum stress corrosion cracking, sustained tensile stress and a relevant environment must coincide with susceptible material. Searching “stress corrosion cracking aluminum” often conflates SCC with general attack; laboratory evidence and service exposure must be distinguished.

7075 aluminum corrosion resistance is also not the same as aluminum corrosion prevention. Aluminum pitting corrosion can occur without the sustained tensile stress required for SCC. “What causes stress corrosion cracking?” is therefore an engineering question about material condition, stress, environment and orientation rather than a single corrosion rating.

3.1. What an SCC Pass Does Not Establish

A batch conductivity acceptance is not evidence that every CNC part underwent a full SCC exposure trial. Likewise, passing a short-transverse coupon test is not a service-life prediction. “How to prevent stress corrosion cracking” has no single temper-only answer: lower the relevant sustained tensile stress where design permits, account for contact and galvanic environments, select the qualified material state, and validate protective measures for the actual application. Do not claim that T73 eliminates all SCC mechanisms or ensures a fixed number of operating years.

4. Match Plate, Bar, and Extrusion to the Correct Specification

A purchase order that says only “7075 aluminum” leaves a critical ambiguity. Rolled plate, rolled or cold-finished bar, and extruded products are governed by different material specifications. Match the actual stock to the proper document before comparing performance numbers.

Starting stockSpecification to checkRFQ decision
Sheet or plateASTM B209/B209M-21a or applicable AMS plate specificationTemper, thickness band, direction, test requirements
Rolled / cold-finished bar, rod or wireASTM B211/B211M-23Section size, temper and bar inspection provisions
Extruded bar, rod, shapes or tubesASTM B221/B221M, applicable order editionExtrusion scope, section limits, temper and properties

The buyer must verify the actual stock temper and available section. A distributor listing for 7075-T651 plate or T7351 plate cannot, by itself, establish the order specification, qualification or delivery date.

Use any AMS material specification only where its scope covers the exact alloy, temper and product form. Do not substitute a plate specification for a bar, or rely on a specification number without checking its revision and scope.

7075 aluminum plate bar and extrusion forms.

The purchasable forms need distinct names. 7075 aluminum sheet and 7075 aluminum plate are rolled products, whereas 7075 aluminum bar, 7075 aluminum round bar and 7075 aluminum flat bar belong to bar product categories. 7075 aluminum extrusion is a different route. Buyers comparing 7075 T6 plate, 7075 T651 plate and 7075 T7351 plate should obtain matching plate certifications; a 7075 T6 bar or 7075 T73 bar cannot be accepted using plate values just because the temper name looks similar.

An RFQ may encounter ASTM B209 aluminum, ASTM B211 aluminum or ASTM B221 aluminum references. Verify the complete designation and edition, not merely the search phrase. ASTM B557 specifies aluminum tensile testing methods, while ASTM E1004 concerns electromagnetic conductivity measurement. AMS 4078 is another specification identifier encountered in aluminum sourcing; do not apply it to a 7075 plate or temper without first checking its actual alloy, product and revision scope.

5. Keep CNC Distortion, Residual Stress, and Flatness Separate

Deep cavities, one-sided stock removal and thin walls can release residual stress and change geometry after unclamping. The temper influences the starting condition; fixture force, toolpath, retained ribs and finishing sequence determine how that condition affects the finished part. Review CNC machining DFM guidelines when planning staged stock removal.

T651 and T7351 both include stretching for stress relief, but neither is distortion-free. Rough critical pockets in stages, retain support, machine opposing faces where geometry allows, and measure after releasing the fixture. The machining route matters as much as the purchasing description.

Machining 7075 aluminum is not simply a cutting-speed decision. The 7075 aluminum machinability of a given billet does not predict whether a large pocket will remain flat. During 7075 aluminum machining, document the fixture reaction, stock removal sequence and free-state datum measurement.

Residual stress measurement can quantify an appropriate test region, and residual stress mapping can reveal spatial differences when a validated method is available. CNC machining simulation and toolpath optimization are useful only after their assumptions are compared with measured geometry and fixture conditions.

5.1. Real Production Case: Controlled Material Removal and Free-State Inspection

In the EPOC CRAFTER instrument housing case, material removal was recorded at approximately 70.37%. Rough machining left 0.5 mm radially and 0.3 mm at the bottom; the semi-finishing stage retained 0.15 mm on critical planes. A soft-jaw setup with three-point base support was followed by datum-based re-fixturing and torque-limited clamps away from the thin walls.

The sequence was first-side layered cavity roughing, retention of peripheral supports and ribs, flipping to machine the opposite datum, release and reinstallation for final features, then deburring. After final unclamping, the part was cleaned and stabilized at 20 ± 1°C for at least two hours. Hole positions were measured by CMM, with a granite surface plate and electronic height gauge used for supplementary flatness checks. The reported acceptance was based on free-state inspection.

This case contains real dimensional results, not a controlled T651-versus-T7351 experiment. Its strongest operational lesson is the inspection condition: a compliant result while fully clamped might conceal springback after release. The actual 0.065 mm flatness and ⌀0.12 mm positional result met limits of 0.10 mm and ⌀0.20 mm respectively. The case does not quantify the relative contribution of temper, toolpath, support or thermal stabilization.

A thin rib can move elastically under clamping and return after release. That motion can shift a datum or hole location even when the material has not yielded. Assess the finished part in the inspection condition required by its drawing.

7075 aluminum machining distortion and fixturing.

6. RFQ and Certification Checks That Change Procurement Risk

7075 CNC part flatness inspection results.

A useful quote specifies alloy, temper, product form, dimensions, test requirements and finished-part acceptance separately. Otherwise suppliers may quote different raw stock under the same shorthand “7075,” making the prices incomparable.

Confirm the required lot identity, specification revision and certificate content at the RFQ stage. Where the application calls for additional mechanical or SCC evidence, state that requirement explicitly. A mill certificate does not replace dimensional inspection of the CNC part. Apply CNC tolerance standards to define inspection and datum requirements.

Before requesting a production quote, fix these details in the RFQ: intended environment and structural load cases; stock geometry and rolling orientation; full temper and specification edition; drawing datums and acceptance criteria; removal volume and thin-wall features; clamping-sensitive inspection conditions; any SCC-related qualification; proposed finish; and sample or production quantity. The RFQ must also state which results belong to the supplied material and which belong to the finished part.

The real case blank volume is 652,800 mm³; at a nominal density of 2.81 g/cm³ its estimated mass is about 1.834 kg. That check supports raw-stock planning, not an invented machining quote. The actual cycle time, material scrap cost and supplier lead time were not provided. Additional flipping and free-state inspection affect routing and must be priced from actual shop operations. EPOC CRAFTER lists precision CNC machining capabilities for this manufacturing conversation.

7075 aluminum suppliers may list different 7075 aluminum stock, lead times and minimum sizes. When evaluating 7075 aluminum price, distinguish the raw product form from 7075 aluminum cost in a finished part. Even a quoted 7075 T6 price does not capture extra setups, material removal, inspection or certification. Compare the actual availability offered by 7075 aluminum bar suppliers and aerospace aluminum suppliers against the same specified product.

A material test report should identify the supplied alloy and temper and the applicable inspections. Aluminum tensile testing documents relevant coupon performance when required, but it does not verify the mounting-face flatness or hole position of the machined assembly. Procurement should request the agreed material certification and finished-part inspection scope rather than treating them as interchangeable.

7. Choose a Temper for Each CNC Application

Part and exposureTemper evaluationDo not skip
Dry fixture or instrument housing with demanding strengthAssess T651 plate or appropriately specified T6 productClamping release, thin-wall flatness and fatigue/load checks
Outdoor fitting under sustained tensile stress and chloride exposureEvaluate qualified T73/T7351 stockSCC evidence, short-transverse orientation and coating
Plate-derived aerospace bracketCompare T651/T7351 by actual plate specification and thicknessSection allowables, inspection and application approval
Extruded profileIdentify a valid extrusion temper/specification firstNo substitution of B211 or B209 limits

For aerospace structures, the governing design and approval requirements control the choice. “Aerospace grade aluminum” is not an acceptance standard. A dry fixture and an exposed structural fitting may require different tempers, even when both use the same 7075 alloy.

A high-load part requires checks for net-section stress, bearing, fatigue, crack tolerance and service exposure. Dimensional acceptance alone does not establish structural suitability. Prototype machining may reveal fixture-sensitive geometry before a production drawing is released. Use rapid prototyping manufacturing to check geometry before repeating the toolpath.

For aerospace grade aluminum, the term “grade” alone is insufficient. Aerospace CNC machining and aerospace precision machining must tie each material state to the drawing, inspection plan and relevant approval. A supplier of aerospace CNC components or aerospace aluminum components may be producing brackets, housings or fixtures with very different loading directions. The choice of temper for 7075 aluminum CNC parts should follow these actual requirements.

Precision CNC machined parts are also vulnerable to datum changes after clamping. In precision aluminum machining, an apparently acceptable hole pattern in a fixture may fail free-state positional tolerance after release. Select the inspection setup alongside the machining route rather than adding it after a purchase order is placed.

8. Emerging Methods Worth Watching

Residual-stress measurement and machining distortion prediction can help identify high-risk features before cutting expensive plate. Their useful output is a testable process change, not a guaranteed flatness value.

Published studies of thin-wall machining and toolpath optimization explore how stock removal and clamping affect deformation. Those results can guide experiments, but models for one geometry or temper cannot be transferred unchanged to another CNC component.

For an engineering trial, measure the same datum and fixturing condition before and after controlled process changes. Record toolpath, setup release, location of removed stock, temperature and measured flatness. This provides a far stronger basis for process choice than an unqualified claim that T7351 always machines flatter than T651.

Current aerospace manufacturing technology studies examine whether verified force and distortion models can improve process planning. X ray diffraction residual stress methods may support localized measurement, while machining process optimization can compare toolpaths under repeatable fixture conditions. Vibration assisted machining is a research option, not proof of improved results on a particular 7075 component.

9. Frequently Asked Questions

9.1. What is 7075 T6 aluminum?

It is 7075 alloy supplied in a solution-heat-treated and artificially aged T6 state. Strength and elongation limits depend on the product standard and cross-section. “7075 T6 aluminum” alone is not a complete drawing or purchase specification.

9.2. How do 7075 T73 vs T7351 and T6 vs T651 differ?

The “51” suffix identifies a stress-relieved-by-stretching route associated with the respective parent heat-treated temper, subject to the authorized designation system. It is not a numerical residual-stress promise. A 7075 T6 vs T651 choice asks about stress relief within a T6-type property family; a 7075 T6 vs T7351 choice also changes the aging/SCC trade-off.

9.3. Can 7075 aluminum be welded?

Conventional fusion welding is generally difficult for 7075 due to hot cracking and property degradation concerns. Welding cannot be assumed acceptable for a critical T6 or T73 component without a qualified joining process and subsequent property verification. Mechanical fastening or another validated joining method may be more practical.

9.4. Can 7075 aluminum be anodized, and does 7075 aluminum rust?

7075 can be anodized subject to the specified finish process and acceptance criteria. Aluminum does not rust like iron, but it corrodes, including localized attack under unfavorable exposure. Anodizing cannot alone establish immunity to stress corrosion cracking or structural suitability. Any post-finish dimensions require their own drawing controls.

9.5. Should a CNC drawing specify T73 instead of T6 whenever corrosion matters?

No. Choose the temper after defining exposure, sustained stress, section size, stock form and applicable qualification requirements. A T73-type selection may reduce SCC susceptibility under relevant conditions, but loss of specified strength can force a section redesign or different acceptance basis. Document the governing material specification, not merely a temper nickname.

Lock service conditions and raw-stock form before selecting the temper. Compare specification limits that actually apply, then define machining release and free-state inspection for the finished geometry.

Scroll to Top
We accept secure online payments Powered by Stripe VISA AMEX UnionPay
Copy link